1296
磁性能表
類別 | 性能 | 剰磁 | 感應強度矯頑力 | 內索矯頑力 | **磁能積 | 工作溫度 | ||||||||
kGs | T | kOe | KA/m | kOe | KA/m | MGOe | Kj/m, | |||||||
Max. | Min. | Max. | Min. | Max. | Min. | Max. | Min. | |||||||
N | N54 | 15.1 | 14 5 | 1.51 | 1.45 | ≥10.5 | ≥836 | ≥11 | ≥836 | 55 | 51 | 438 | 406 | ≤80 |
N52 | 14.8 | 14.2 | 1.48 | 1.42 | ≥10.5 | ≥836 | ≥11 | ≥836 | 53 | 49 | 422 | 390 | ≤80 | |
N50 | 14.5 | 14 | 1.45 | 1.4 | ≥11.0 | ≥876 | ≥11 | ≥876 | 51 | 47 | 406 | 374 | ≤80 | |
N48 | 14 3 | 137 | 1.43 | 1.37 | ≥11.0 | ≥876 | ≥12 | ≥955 | 49 | 45 | 390 | 358 | ≤80 | |
N45 | 13.8 | 13.2 | 1.38 | 1.32 | ≥11.0 | ≥876 | ≥12 | ≥955 | 46 | 42 | 366 | 334 | ≤80 | |
N42 | 13.5 | 129 | 1.35 | 1.29 | ≥11.0 | ≥876 | ≥12 | ≥955 | 44 | 40 | 350 | 318 | ≤80 | |
N40 | 13.2 | 12.6 | 1.32 | 1.26 | ≥11.0 | ≥876 | ≥12 | ≥955 | 41 | 38 | 334 | 302 | ≤80 | |
N38 | 13 | 122 | 1.3 | 1.22 | ≥11.0 | ≥876 | ≥12 | ≥955 | 40 | 36 | 318 | 287 | ≤80 | |
N35 | 12.2 | 11.7 | 1.22 | 1.17 | ≥10.9 | ≥868 | ≥12 | ≥955 | 36 | 33 | 287 | 263 | ≤80 | |
N33 | 11.7 | 11.3 | 1.17 | 1.13 | ≥10.5 | ≥836 | ≥12 | ≥955 | 34 | 31 | 271 | 247 | ≤80 | |
N30 | 11.3 | 10.8 | 1.13 | 1.08 | ≥10.0 | ≥796 | ≥12 | ≥955 | 31 | 28 | 247 | 223 | ≤80 | |
M | N52M | 14.8 | 14.2 | 1.48 | 1.42 | ≥13.3 | ≥1059 | ≥l4 | ≥1114 | 43 | 49 | 422 | 390 | ≤100 |
N50M | 14.5 | 14.0 | 1.45 | 1.40 | ≥13.1 | ≥1043 | ≥14 | ≥1114 | 41 | 47 | 406 | 374 | ≤100 | |
N48M | 14.3 | 13.7 | 1.43 | 1.37 | ≥12.8 | ≥1019 | ≥14 | ≥1114 | 49 | 45 | 390 | 358 | ≤100 | |
N45M | 13.8 | 13.2 | 1.38 | 1.32 | ≥12.4 | ≥987 | ≥14 | ≥1114 | 46 | 42 | 366 | 334 | ≤100 | |
N42M | 13.5 | 12.9 | 1.35 | 1.29 | ≥12.1 | ≥963 | ≥14 | ≥1114 | 44 | 40 | 350 | 318 | ≤100 | |
N40M | 13.2 | 126 | 1.32 | 1.26 | ≥11.8 | ≥939 | ≥14 | ≥1114 | 41 | 38 | 334 | 302 | ≤100 | |
N38M | 13 | 12.2 | 1.3 | 1.22 | ≥11.7 | ≥915 | ≥14 | ≥1114 | 40 | 36 | 318 | 287 | ≤100 | |
N35M | 12.2 | 11.7 | 1.22 | 1.17 | ≥10.9 | ≥868 | ≥14 | ≥1114 | 36 | 33 | 287 | 263 | ≤100 | |
H | N50H | 14.5 | 14.0 | 1.45 | 1.40 | ≥12.9 | ≥1027 | ≥16 | ≥1274 | 51 | 47 | 406 | 374 | ≤120 |
N48H | 14.3 | 13.7 | 1.43 | 1.37 | ≥12.7 | ≥1011 | ≥16 | ≥1274 | 49 | 45 | 390 | 358 | ≤120 | |
N46H | 14 | 13.4 | 1.4 | 1.34 | ≥12.5 | ≥995 | ≥17 | ≥1353 | 47 | 43 | 374 | 342 | ≤120 | |
N44H | 13.7 | 13 1 | 1.37 | 1.31 | ≥12.3 | ≥979 | ≥17 | ≥1353 | 45 | 41 | 358 | 326 | ≤120 | |
N42H | 13.5 | 129 | 1.35 | 1.29 | ≥12.1 | >963 | ≥17 | ≥1353 | 44 | 40 | 350 | 318 | ≤120 | |
N40H | 13.2 | 12.6 | 1.32 | 1.26 | ≥11.8 | ≥939 | ≥17 | ≥1353 | 42 | 38 | 334 | 302 | ≤120 | |
N38H | 130 | 122 | 1.3 | 1.22 | ≥11.5 | ≥915 | ≥17 | ≥1353 | 40 | 36 | 318 | 287 | ≤120 | |
N35H | 12.4 | 11.7 | 1.24 | 1.17 | ≥11.0 | ≥876 | ≥17 | ≥1353 | 37 | 33 | 295 | 263 | ≤120 | |
N33H | 11.7 | 11.3 | 1.17 | 1.13 | ≥10.5 | ≥836 | ≥17 | ≥1353 | 34 | 31 | 271 | 247 | ≤120 | |
SH | N45SH | 14 | 13.4 | 1.4 | 1.34 | ≥12.5 | ≥995 | ≥20 | ≥1592 | 47 | 43 | 374 | 342 | ≤150 |
N44SH | 13.7 | 13.1 | 1.37 | 1.31 | ≥12.3 | ≥979 | ≥20 | ≥1592 | 45 | 41 | 358 | 362 | ≤150 | |
N42SH | 13.5 | 12.9 | 1.35 | 1.29 | ≥12.1 | ≥963 | ≥20 | ≥1592 | 44 | 40 | 350 | 318 | ≤150 | |
N40SH | 13.2 | 126 | 1.32 | 1.26 | ≥11.8 | ≥939 | ≥20 | ≥1592 | 42 | 38 | 334 | 302 | ≤150 | |
N38SH | 12.9 | 12.2 | 1.29 | 1.22 | ≥11.5 | ≥915 | ≥20 | ≥1592 | 40 | 36 | 318 | 287 | ≤150 | |
N35SH | 124 | 11.7 | 1.24 | 1.17 | ≥11.0 | ≥876 | ≥20 | ≥1592 | 37 | 33 | 295 | 263 | ≤150 | |
N33SH | 12.1 | 11.4 | 1.21 | 1.14 | ≥10.7 | ≥852 | ≥20 | ≥1592 | 35 | 31 | 279 | 247 | ≤150 | |
UH | N42UH | 13.5 | 12.9 | 1.35 | 1.29 | ≥12.1 | ≥963 | ≥25 | 1990 | 44 | 40 | 350 | 318 | ≤180 |
N40UH | 132 | 126 | 1.32 | 1.26 | ≥11.8 | ≥939 | ≥25 | 1990 | 42 | 38 | 334 | 302 | ≤180 | |
N38UH | 12.9 | 12.2 | 1.29 | 1.22 | ≥11.5 | ≥915 | ≥25 | 1990 | 40 | 36 | 318 | 287 | ≤180 | |
N35UH | 124 | 11.7 | 1.24 | 1.17 | ≥11.0 | ≥876 | ≥25 | 1990 | 37 | 33 | 295 | 263 | ≤180 | |
N33UH | 12.1 | 11.4 | 1.21 | 1.14 | ≥10.7 | ≥852 | ≥25 | 1990 | 35 | 31 | 379 | 247 | ≤180 |
物理特性
項目 | 參數 | 參考值 |
輔助磁性能 | 剩磁溫度系數 | -0.08~-0.12 |
(a (Br) ) /(%/K) | ||
內稟矯頑力溫度系數 | -0.42~-0.07 | |
(β (Hcj) ) /(%/K) | ||
居里溫度 | 310-380 | |
(Tc) /K | ||
回復磁導率 | 1.05 | |
(μ rec) [-] | ||
機械物理特性 | 密度(g/m3) | 7.50-7.70 |
維式硬度/ (Hv) | 650 | |
電阻率/ (μ Ω om) | 1.4 | |
抗壓強度/ (MPa) | 1050 | |
抗拉強度/ (MPa) | 80 | |
抗彎強度/ (MPa) | 290 | |
耕專導豹(W/(mok)) | 6~8 | |
楊氏模量/ (GPa) | 160 | |
熱膨脹系數(垂直于取向方向)/(10-6/K) | -1.5 | |
熱膨脹系數(平行于取向方向)(10-6/K) | 6.5 | |
磁性性能參數及換算表
參數及表示 | 國際單位 | 單位換算 |
磁感應強度B | T | 1T=1Vs/m2=10kGs |
磁極化強度J | T | 1T=1Vs/m2=10kGs |
磁場強度H | KA/m | 1KA/m=4ΠOe≈12.57Oe |
磁能積(BH) | KJ/m3 | 1KA/m3=0.126MGOe |
磁通Φ | Wb | 1Wb=1Vs=108Mx |
產品尺寸
類別 | 圖示 | 規格 | 推薦尺寸/mm | 極限尺寸/mm |
方塊類 | L | ≤180 | ≤220 | |
W | ≤120 | ≤150 | ||
T | ≤60 | ≤80 | ||
圓柱類 | D | ≤150 | ≤220 | |
T | ≤60 | ≤80 | ||
圓環類 | D | ≤120 | ≤160 | |
d | ≤80 | ≤100 | ||
T | ≤45 | ≤65 | ||
瓦片類 | L | ≤180 | ≤220 | |
W | ≤120 | ≤150 | ||
T | ≤60 | ≤80 | ||
a | 0~180℃ |
表面處理
釹鐵硼機體極易被腐蝕,為了克服此缺陷,常常對其表面進行涂覆。通常采用的方法有鍍藍白鋅、彩鋅;鍍鎳、雙層鎳、鎳錫、鎳銅鎳;鍍環氧樹脂; (臨時保護)磷化等。
表面處理指標
Coating perfomace | Zn | Color Zn | Ni | Double Ni | NiSn | NiCuNi | ElectrolessNi | Epoxy | Passivation |
Color | white | multicolour | silver | silver | silver | silver | silver | black | silver |
Thickness(μm) | 5-10 | 5-15 | 10-15 | 15-20 | 10-20 | 10-25 | 10-20 | 25-30 | 1-5 |
Pressure Cooker Test (120℃. 2atm,100%RH) | >15hr | >24hr | >48hr | >48hr | >72hr | >48hr | >48hr | >24hr | >4hr |
Salt Spray lest | >15hr | >24hr | >24hr | > 24hr | >48hr | >24hr | >48hr | > 500hr | >8hr |